Operation Steps of Medium Frequency Melting Furnace before Cast Steel 1. If the melting furnace is electrified: power on for 4 ~ 8 min to supply 60% power of intermediate frequency furnace, and gradually increase the power to the maximum value after the current impact stops. 2. Ramming material for melting: as the lower part of the pot melts, pay attention to tamping at any time to prevent "bridging", and continue to add furnace charge. 3. Slagging: after most of the furnace charge is melted, slagging material (mass ratio: lime powder: fluorspar powder = 2:1) is added to cover the molten steel, and the amount of slag forming material is 1% ~ 1.5% of the weight of liquid steel. 4. Sampling and slagging: when about 95% of the charge is melted, the steel sample is taken for analysis, and the remaining 5% of the charge is added into the furnace. After all the burden is dissolved, the power is reduced to 40% ~ 60%, and the slag is removed by dumping and new slag is made. ...